0%

Table of Contents

I. Gold and Silver Ink Blending 1. BOPP/PE series (LP code) blending method for turquoise gold: ① Take a clean empty bucket, then pour out 10kg of JR-LP-22 transparent yellow; ② Place it on the mixer and stir, then add 2kg of XL-10A silver paste; When adding the silver paste, add it slowly and evenly in small portions, do not add a spoonful of silver paste at once into the ink; ③ After adding the silver paste, use the mixer to fully stir for 5 minutes, the mixer speed should be controlled between H30 - H40; After thorough stirring, filter the prepared ink before using (to prevent dark lines when printing over a large area); 2. PET/BOPA series (LA code) series LA turquoise gold blending method: ① Take a clean empty bucket, then pour out 10kg of MG-DF-R4350 transparent yellow; ② Place it on the mixer and stir, then add 2kg of XL-10A silver paste; When adding the silver paste, add it slowly and evenly in small portions, do not add a spoonful of silver paste at once into the ink; ③ After adding the silver paste, use the mixer to fully stir for 5 minutes, the mixer speed should be controlled between H30 - H40; After thorough stirring, filter the prepared ink before using (to prevent dark lines when printing over a large area); 3. BOPP/PE series (LP code) gold powder ink blending method: ① Take a clean empty bucket, then pour out 10kg of JR-LP gold-tinted ink; ② Place it on the mixer and stir, then add 2kg of turquoise powder; When adding the turquoise powder, add it slowly and evenly in small portions, do not add a spoonful of turquoise powder at once into the ink; ③ After adding the turquoise powder, use the mixer to fully stir for 5 minutes, the mixer speed should be controlled between H30 - H40; After thorough stirring, filter the prepared ink before using (to prevent dark lines when printing over a large area); Additionally: LA gold powder ink blending method is the same as LP gold powder ink blending method, just replace JR-LP gold-tinted ink with JR-LA gold-tinted ink. 4. BOPP/PE series (LP code) silver ink blending method: ① Take a clean empty bucket, then pour out 10kg of JR-LP gold-tinted ink; ② Place it on the mixer and stir, then add 2kg of XL-239 silver paste; When adding the silver paste, add it slowly and evenly in small portions, do not add a spoonful of silver paste at once into the gold-tinted ink; ③ After adding the silver paste, use the mixer to fully stir for 5 minutes, the mixer speed should be controlled between H30 - H40; After thorough stirring, filter the prepared ink before using (to prevent dark lines when printing over a large area); Additionally: LA silver ink blending method is the same as LP silver ink blending method, just replace JR-LP gold-tinted ink with JR-LA gold-tinted ink. II. Pearl Ink Blending 1. BOPP/PE series (LP code) pearl white blending method: ① Take a clean empty bucket, then pour out 10kg of JRLP gold-tinted ink; ② Place it on the mixer and stir, then add 1.5kg of Oke Pearl White - 1120#; When adding the pearl powder, add it slowly and evenly in small portions, do not add a spoonful of pearl powder at once into the gold-tinted ink; ③ After adding the pearl powder, use the mixer to fully stir for 5 minutes, the mixer speed should be controlled between H20–H30 (too fast a speed will damage the pearl effect); After thorough stirring, filter the prepared ink before using (to prevent dark lines when printing over a large area); Additionally: LA pearl white blending method is the same as LP pearl white blending method, just replace JR-LP gold-tinted ink with JR-LA gold-tinted ink. 2. Interference purple blending method: (for anti-counterfeiting of GBL products) ① Take a clean empty bucket, then pour out 10kg JRLP gold oil; ② Place it on the mixer and stir, then add 2.5kg Oke interference purple powder; When adding pearlescent powder, add the interference purple powder slowly and evenly in small amounts, and do not add one spoon of interference purple powder all at once to the gold oil; ③ After adding the interference purple powder, use the mixer to stir thoroughly for 5 minutes, and control the mixer speed between H20 - H30 (if the stirring speed is too fast, it will damage the pearlescent effect); After thorough stirring, filter the prepared ink before using (to prevent dark lines when printing over a large area); 3. Table printing (JR) pearlescent white blending method: ① Take a clean empty bucket, then pour out 10kg JR-8199D high-temperature resistant gold oil; ② Place it on the mixer and stir, then add 1.5kg Oke pearlescent powder - 1120#; When adding pearlescent powder, add the pearlescent powder slowly and evenly in small amounts, and do not add one spoon of pearlescent powder all at once to the gold oil; ③ After adding the pearlescent powder, use the mixer to stir thoroughly for 5 minutes, and control the mixer speed between H20 - H30 (if the stirring speed is too fast, it will damage the pearlescent effect); After thorough stirring, filter the prepared ink before using (to prevent dark lines when printing over a large area); Three. Blending of transparent ink 1. Blending method of transparent ink for PET/BOPA series (LA code) (except transparent dark blue): ① Take a clean empty bucket, then pour out 10kg JRLA gold oil; ② Place it on the mixer and stir, then add 1kg dye color powder; When adding dye color powder, add the dye color powder slowly and evenly in small amounts, and do not add one spoon of dye color powder all at once to the gold oil; ③ After adding silver paste, use the mixer to stir thoroughly for 5 minutes, and control the mixer speed between H30 - H40; After thorough stirring, filter the prepared ink before using (to prevent printing plate blocking due to incomplete dissolution of some dyes) Additionally: The blending method of non-phenolic transparent ink is the same as that of LA transparent ink, just replace JR LA gold oil with YZJ non-phenolic gold oil; 2. Blending method of transparent dark blue ink for PET/BOPA series (LA code): ① Take a clean empty bucket, then pour out 10kg JRLA gold oil; ② Place it on the mixer and stir, then add 0.5kg ethanol solvent; ③ Then add 0.6kg - 0.7kg dye color powder; When adding dye color powder, add the dye color powder slowly and evenly in small amounts, and do not add one spoon of dye color powder all at once to the gold oil; ④ After adding dye color powder, use the mixer to stir thoroughly for 5 minutes, and control the mixer speed between H30 - H40; Then add an appropriate amount (about 4kg) of solvent, continue stirring for 5 minutes; After thorough stirring, filter the prepared ink before using (to prevent printing plate blocking due to incomplete dissolution of some dyes) Additionally: The blending method of non-phenolic transparent dark blue ink is the same as that of LA transparent dark blue ink, just replace JR LA gold oil with YZJ non-phenolic gold oil; 

Personal opinion, only for reference.

Michael Thompson

Michael Thompson

Michael Thompson is Chengheng Plastic Machinery’s Lead Service Technician for the United States. He’s based in Houston, Texas and is responsible for installation, maintenance, and repair of our bag making and printing machines across the country. Michael has over 15 years of hands-on experience in machine servicing and troubleshooting, and holds several certifications in industrial automation. He’s known for his quick response times and commitment to minimizing downtime for our clients. Michael also develops and delivers on-site training for operators to ensure they can maximize the efficiency of their equipment.
Previous Choosing a 7 Layer Co-Extrusion Film Blowing Machine: Working Requirements and Integration Fit
Next Methods for Formulating Specialty Inks Used in Flexible Packaging